10 years 11 months ago - 10 years 11 months ago #2705 by Mr Nima Rahati
Flexibility was created by Mr Nima Rahati
HI,
Issue
Process : magnet round copper wire
Problem : fault in flexibility test (mandrel or 1D test), cracking of coating after bending.
Information
wire size: 1.20 mm
enamel type : polyester imide (2L)
oven type : horizontal
oven temperature: 580 C
anneal temperature : 550 C
speed : 85 m/min
number of passes : 22 - 23 passes
tangent delta : good
elongation :good
Thanks a lot for any advice to resolve this issue.
Nima
Issue
Process : magnet round copper wire
Problem : fault in flexibility test (mandrel or 1D test), cracking of coating after bending.
Information
wire size: 1.20 mm
enamel type : polyester imide (2L)
oven type : horizontal
oven temperature: 580 C
anneal temperature : 550 C
speed : 85 m/min
number of passes : 22 - 23 passes
tangent delta : good
elongation :good
Thanks a lot for any advice to resolve this issue.
Nima
Last edit: 10 years 11 months ago by Mr Nima Rahati. Reason: editing
Please Log in to join the conversation.
- Richard Burke
- Offline
- Senior Boarder
Less More
- Posts: 64
- Thank you received: 8
10 years 11 months ago - 10 years 10 months ago #2712 by Richard Burke
Replied by Richard Burke on topic Re: Flexibility
Sounds like over cured insulation to me. What are your cut through values?
Also you say the tan delta is good but where is in the range of what is good?
Also you say the tan delta is good but where is in the range of what is good?
Last edit: 10 years 10 months ago by Peter J Stewart-Hay.
Please Log in to join the conversation.
- Mr Nima Rahati
- Topic Author
- Offline
- Junior Boarder
Less More
- Posts: 25
- Thank you received: 1
10 years 11 months ago - 10 years 10 months ago #2714 by Mr Nima Rahati
Replied by Mr Nima Rahati on topic Re: Flexibility
Thank you for your reply
According your request ;
1- For cut through standard value is 300 c at 2 min. And our cut. was 320
2- For tangent delta standard range for this size is 195 to 210 and our actual values in different oven regulations (different temperatures and speeds) was 197.4, 200.7, 211.4, 214.6, 200.8 and all of them not OK in flexibility.
Thanks.
According your request ;
1- For cut through standard value is 300 c at 2 min. And our cut. was 320
2- For tangent delta standard range for this size is 195 to 210 and our actual values in different oven regulations (different temperatures and speeds) was 197.4, 200.7, 211.4, 214.6, 200.8 and all of them not OK in flexibility.
Thanks.
Last edit: 10 years 10 months ago by Peter J Stewart-Hay.
Please Log in to join the conversation.
- Richard Burke
- Offline
- Senior Boarder
Less More
- Posts: 64
- Thank you received: 8
10 years 10 months ago #2724 by Richard Burke
Replied by Richard Burke on topic Cracking insulation
Isn't the standard test a 3X mandrel? Assuming the cracks in the insulation are not being caused by problems with the bare wire (do a 1X test of the bare wire and check surface quality) I still think that you have an over cured insulation. You can check this by increasing the speed slightly (easier than chaning curing temperatures and air flow) while maintaining dimensions. Test the wire after doing this and see if it cracks
Please Log in to join the conversation.
- Mr Prashant Sankhe
- Offline
- Fresh Boarder
Less More
- Posts: 3
- Thank you received: 1
10 years 10 months ago #2725 by Mr Prashant Sankhe
Replied by Mr Prashant Sankhe on topic Re: Flexibility
Dear Nima
I also believe that its an over cured wire . For giving solution to this problem i would like to know few things.
1) You are checking tangent delta with cooling to heating method or heating to cooling method ?
2) What does your enamel manufacturers technical datasheet says with regards to the tangent delta value ?
3) What is the peel value and springiness value of enamel wire against standard requirement ?
One more additional thing you have to check is surface condition of bare wire before entering application area. It should be bright and clean.
All of the above you can check homogeneity of enamel insulation if you have that testing facility.
Best Luck
I also believe that its an over cured wire . For giving solution to this problem i would like to know few things.
1) You are checking tangent delta with cooling to heating method or heating to cooling method ?
2) What does your enamel manufacturers technical datasheet says with regards to the tangent delta value ?
3) What is the peel value and springiness value of enamel wire against standard requirement ?
One more additional thing you have to check is surface condition of bare wire before entering application area. It should be bright and clean.
All of the above you can check homogeneity of enamel insulation if you have that testing facility.
Best Luck
Please Log in to join the conversation.
- Ing Nicola Restaino
- Offline
- Fresh Boarder
Less More
- Posts: 13
- Thank you received: 0
10 years 10 months ago #2728 by Ing Nicola Restaino
Replied by Ing Nicola Restaino on topic Re: Flexibility
I had the same problem in two vertical Sicme Ovens.
The problem was in one of them I passed the mandrel test, in the other one no.
The only thing different was the adjustements of the oven, I mean Temperature and Flow air.
Regards
Nicola
The problem was in one of them I passed the mandrel test, in the other one no.
The only thing different was the adjustements of the oven, I mean Temperature and Flow air.
Regards
Nicola